PTFE/MoS₂ Test Data: What the XRD and Sliding-Wear Results Mean

PTFE/MoS₂ Test Data: What the XRD and Sliding-Wear Results Mean

未分类 Updated

PEFLON’s authorized PTFE/MoS₂ test series gives two useful but different answers. The GB/T 3960 sliding-wear results show that every tested MoS₂-filled composition wore less than unfilled PTFE under that test, with the lowest reported value at 15 wt% rather than 20 wt%. The XRD series shows the PTFE characteristic peak and additional peaks assigned in the source to MoO₃ formed during sintering. Together, the results support testing 5%, 10%, 15% and 20% options against the real counterface and duty cycle. They do not prove that one loading is universally best.

What PEFLON Tested

The PEFLON evidence package contains a controlled loading series rather than a single filled sample. For sliding wear, it compares unfilled PTFE with 5, 10, 15 and 20 wt% MoS₂. For phase analysis, it compares unfilled PTFE with the filled compounds and reports the principal diffraction positions used in the original interpretation.

This design matters because it exposes the shape of the response. If the evidence had compared only unfilled PTFE with 20% MoS₂, a buyer might conclude that more filler always means less wear. The five-point series shows otherwise. The value improves through 15% and then rises at 20% under the reported method.

PEFLON currently supplies 5%, 10%, 15% and 20% MoS₂-filled PTFE. Availability does not remove the need for qualification: the choice among those four options still depends on the mating surface, pressure, speed, temperature, atmosphere, geometry and acceptable wear mechanism.

The GB/T 3960 Wear Series Shows an Optimum, Not a Straight Line

The central result is that all four filled compositions measured below unfilled PTFE, but the ranking was not monotonic. The reported wear value fell from 7.6 for unfilled PTFE to 1.9 at 15 wt% MoS₂, then increased to 2.8 at 20 wt%.

GB/T 3960 sliding wear results for PTFE with different MoS2 loadings
Test composition Reported wear value Result within this series
Unfilled PTFE 7.6 ×10−7 cm³/(N·m) Reference
5 wt% MoS₂ 4.9 ×10−7 cm³/(N·m) Below unfilled PTFE
10 wt% MoS₂ 4.0 ×10−7 cm³/(N·m) Below the 5% test point
15 wt% MoS₂ 1.9 ×10−7 cm³/(N·m) Lowest reported value
20 wt% MoS₂ 2.8 ×10−7 cm³/(N·m) Higher than the 15% test point

The method named in the source is GB/T 3960-2016, Plastics—Test method for friction and wear by sliding. The official SAMR record identifies it as a current Chinese national standard. The table above reproduces the PEFLON-reported results; it does not substitute a different test method or combine numbers from external publications.

Why the 15% Result Does Not Make 15% Universally Best

The 15% composition is the best performer only within this PEFLON test series. Wear is a system response, not a standalone material constant. Changing the counterface, pressure, velocity, temperature, humidity, atmosphere, surface finish, motion pattern or test duration can change both the absolute wear rate and the relative ranking.

This limitation is not a reason to ignore the data. It tells the buyer how to use it correctly. The curve is strong evidence against selecting 20% simply because it contains more MoS₂. It is also a rational basis for including 15% in an application trial. It is not evidence that 15% will deliver the longest life in every seal, bushing, bearing or guide component.

The official ASTM D3702 page makes the same general qualification point for self-lubricated rubbing materials: when test conditions change, wear rates and relative material rankings may change. ASTM D3702 is not presented here as the method used by PEFLON; GB/T 3960 is the reported method. It is cited only to show why tribology results must stay tied to their conditions.

How the Counterface Can Change Filled-PTFE Wear

The counterface can change both the measured wear rate and which MoS₂ loading ranks first. Its material, hardness, surface finish and condition influence transfer-film formation, local contact stress and abrasion at the sliding interface. A result obtained against one counterface therefore cannot approve the same compound against a different metal, coating or surface finish.

For qualification, record the counterface material and finish with the PTFE/MoS₂ composition, load, speed, temperature and duration. If the application changes any of those variables, repeat the comparison rather than assuming the 15% result will remain the optimum. This is the practical reason the PEFLON series is a screening basis, not a universal service-life table.

What the XRD Series Shows

The XRD evidence confirms that the filled compounds do not reproduce the unfilled PTFE pattern alone. Unfilled PTFE showed the characteristic peak reported at 2θ = 18.1°. In the PTFE/MoS₂ compounds, the source also reports peaks at 2θ = 26.4° and 54.5° and assigns them to MoO₃ formed by partial oxidation of MoS₂ during sintering.

Redrawn XRD phase analysis chart for PTFE and MoS2 compounds
Reported position Source interpretation Practical reading
2θ = 18.1° PTFE characteristic peak Reference feature of the PTFE matrix
2θ = 26.4° Additional peak assigned to MoO₃ Loading and thermal history should be considered together
2θ = 54.5° Additional peak assigned to MoO₃ Supports the source’s partial-oxidation interpretation

The figure is a faithful redraw of the authorized chart, not raw instrument output. Each trace is offset vertically so that the peak positions remain readable. The offsets therefore must not be interpreted as absolute intensity differences among the compositions.

What the XRD Evidence Does Not Prove

The XRD chart does not by itself establish coefficient of friction, wear life, tensile strength or service temperature. It also does not prove that the observed phase assignment is the sole cause of the wear ranking. Phase analysis and tribological testing answer different questions: XRD describes crystalline features in the tested material, while the sliding-wear test measures the response of a material pair under a defined mechanical procedure.

The evidence is still commercially useful. It shows why the sintering process should be recorded when a trial is repeated, especially if a customer compares parts made by different processors or production cycles. A change in heating history should not be treated as irrelevant simply because the nominal MoS₂ percentage stayed the same.

For the broader mechanism, the Society of Tribologists and Lubrication Engineers explains that layered solids such as molybdenum disulfide can accommodate shear between atomic layers. That general mechanism helps explain why MoS₂ is considered as a solid lubricant, but it does not replace compound-specific testing.

How to Turn the Test Series Into a Qualification Plan

A useful qualification plan starts with the friction pair, not the filler percentage. Send the counterface material and finish, the contact pressure or applied load, sliding speed, temperature, atmosphere or process medium, motion type, target life and acceptable dimensional change. Add the requested supply form and drawing when the compound will be machined into a finished part.

  1. Define the failure mode. Decide whether the current problem is wear, creep, friction instability, heat generation, dimensional loss or damage to the mating surface.
  2. Choose a short loading set. Use the PEFLON series to avoid assuming that the highest loading is automatically the strongest candidate. Depending on the application, compare 10%, 15% and 20%, or begin with 5% when lower filler content is preferred.
  3. Hold the process history. Keep molding, sintering and machining conditions traceable so that a material change is not confused with a process change.
  4. Reproduce the contact. Use the intended counterface, surface finish, pressure, speed, temperature and environment as closely as practical.
  5. Approve the complete part. A low material wear value does not automatically approve leakage, dimensional stability, mating-surface wear or assembly performance.

For the available forms and the commercial inquiry path, use the PEFLON MoS₂ filled PTFE product page. When the filler family is still undecided, compare the wider PEFLON modified PTFE range before narrowing the trial.

When Another Filled PTFE System May Be a Better Starting Point

MoS₂ is not a default answer for every filled-PTFE application. If the central requirement is electrical behaviour, chemical compatibility with a particular medium, mating-surface protection or a different balance of creep and strength, another filler system may deserve the first trial. A buyer should compare the complete material pair and environment rather than transferring a solid-lubricant reputation directly into a finished-part decision.

The existing graphite vs MoS₂ vs PTFE solid-lubricant guide addresses the chemistry-level distinction. The PTFE grade-selection guide helps separate resin form, processing route and filled-compound decisions. Neither page replaces the PEFLON test evidence reported here.

Frequently Asked Questions

Does more MoS₂ always reduce PTFE wear?

No. In the authorized PEFLON series, the reported wear value was lowest at 15 wt% and increased at 20 wt%.

Is 15% MoS₂ filled PTFE available from PEFLON?

Yes. PEFLON supplies 15% MoS₂ filled PTFE as well as 5%, 10% and 20% options. Application qualification is still required.

Was ASTM D3702 used for the PEFLON wear values?

No. The PEFLON source identifies GB/T 3960-2016 as the test method. ASTM D3702 is cited only for its explanation that changing tribology conditions can change material rankings.

What does the 18.1° XRD peak represent?

The authorized source identifies 2θ = 18.1° as the characteristic PTFE peak in the tested series.

Do the 26.4° and 54.5° peaks prove better wear resistance?

No. The source assigns these peaks to MoO₃ associated with partial oxidation during sintering, but XRD alone does not prove a wear mechanism or service-life improvement.

Can these wear values be used as product specifications?

No. They are reported test results for the authorized series, not universal specification limits. Request the applicable commercial documentation and reproduce the intended service conditions.

Request a Loading Trial

Send PEFLON the counterface, load, speed, temperature, atmosphere or process medium, target life, dimensions and required form. The technical team can use those inputs to choose a practical comparison among the available 5%, 10%, 15% and 20% MoS₂ options and respond within 24 hours with the next qualification step.

By Zola Zhao, Technical Engineer.